公司信息及水印
牌号简介 About |
---|
LEXAN FST3002树脂是MVR为8的无卤阻燃PC共聚树脂,适用于注塑成型。该树脂符合EN45545 R6 HL2标准,是列车内部应用(R6类)的理想选择。提供不透明色 LEXAN FST3002 resin is a halogen-free flame retardant PC Copolymer Resin with MVR of 8, suitable for injection molding. This resin is EN45545 R6 HL2 compliant and an ideal candidate for train interior applications (category R6). Available in opaque colors |
技术参数 Technical Data | |||
---|---|---|---|
物理性能 PHYSICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
密度 Density |
1.22 | g/cm³ | ASTM D792 |
熔体质量流动速率 Melt Flow Rate |
|||
300℃,1.20kg 300℃,1.20kg |
9.0 | g/10min | ASTM D1238 |
熔体体积流动速率 Melt Volume Rate |
|||
300℃,1.2 kg 300℃,1.2 kg |
8.00 | cm³/10min | ISO 1133 |
收缩率 Shrinkage rate |
|||
MD MD |
0.50 到 0.70 | % | |
TD TD |
0.50 到 0.70 | % | |
机械性能 MECHANICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
拉伸模量 Tensile modulus |
|||
-- -- 2 |
MPa | ASTM D638 | |
-- -- |
MPa | ISO 527-1-2 | |
拉伸强度 tensile strength |
|||
屈服 yield 3 |
MPa | ASTM D638 | |
屈服 yield |
MPa | ISO 527-2/50 | |
断裂 fracture 3 |
MPa | ASTM D638 | |
断裂 fracture |
MPa | ISO 527-2/50 | |
拉伸应变 Tensile strain |
|||
屈服 yield 3 |
% | ASTM D638 | |
屈服 yield |
% | ISO 527-2/50 | |
断裂 fracture 3 |
% | ASTM D638 | |
断裂 fracture |
% | ISO 527-2/50 | |
弯曲模量 Bending modulus |
|||
50 mm跨距 50 mm span 4 |
MPa | ASTM D790 | |
-- -- 5 |
MPa | ISO 178 | |
弯曲强度 bending strength |
|||
-- -- 5 , 6 |
MPa | ISO 178 | |
屈服,50 mm跨度 Yield, 50 mm span 4 |
MPa | ASTM D790 | |
冲击性能 IMPACT |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
简支梁缺口冲击强度 Charpy Notched Impact Strength 7 |
|||
-30℃ -30℃ |
kJ/m² | ||
23℃ 23℃ |
kJ/m² | ||
简支梁无缺口冲击强度 Charpy Unnotch Impact strength 7 |
|||
-30℃ -30℃ |
|||
23℃ 23℃ |
|||
悬臂梁缺口冲击强度 Impact strength of cantilever beam notch |
|||
-30℃ -30℃ |
J/m | ASTM D256 | |
23℃ 23℃ |
J/m | ASTM D256 | |
-30℃ -30℃ 8 |
kJ/m² | ISO 180-1A | |
23℃ 23℃ 8 |
kJ/m² | ISO 180-1A | |
悬臂梁无缺口冲击强度 Notched impact strength of cantilever beam 8 |
|||
-30℃ -30℃ |
|||
23℃ 23℃ |
|||
装有测量仪表的落镖冲击 Dart impact equipped with measuring instruments |
|||
23℃,Total Energy 23℃,Total Energy |
J | ASTM D3763 | |
-- -- |
J | ISO 6603-2 | |
热性能 THERMAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
热变形温度 Hot deformation temperature |
|||
0.45 MPa,未退火,3.2 mm 0.45 MPa, unannealed, 3.2 mm |
℃ | ASTM D648 | |
0.45 MPa,未退火,4.0 mm,64 mm跨距 0.45 MPa, unannealed, 4.0 mm, 64 mm span 9 |
℃ | ISO 75-2/Bf | |
1.8 MPa,未退火,3.2 mm 1.8 MPa, unannealed, 3.2 mm |
℃ | ASTM D648 | |
1.8 MPa,未退火,4.0 mm,64 mm跨距 1.8 MPa, unannealed, 4.0 mm, 64 mm span 9 |
℃ | ISO 75-2/Af | |
维卡软化温度 Vicat Softening Temp |
|||
-- -- |
℃ | ASTM D1525 10 | |
-- -- |
℃ | ISO 306/A120 | |
线性热膨胀系数 Linear coefficient of thermal expansion |
|||
MD:-40~40℃ MD:-40~40℃ |
1/℃ | ||
TD:-40~40℃ TD:-40~40℃ |
1/℃ | ||
阻燃性能 FLAME CHARACTERISTICS |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
Fire Safety Hazard Level(Requirement set R6) Fire Safety Hazard Level(Requirement set R6) |
EN 45545-2 | ||
Smoke Toxicity - CITG(8 min)(3.00 mm) Smoke Toxicity - CITG(8 min)(3.00 mm) 11 |
ISO 5659-2 | ||
放热 exothermic 11 |
|||
MAHRE,3.00 mm MAHRE,3.00 mm 11 |
kW/m² | ISO 5660-1 | |
烟雾密度 Smoke density 11 |
|||
DS-4:3.00 mm DS-4:3.00 mm |
|||
VOF4:3.00 mm VOF4:3.00 mm |
备注 |
---|
2. 50 mm/min |
3. 类型 1, 50 mm/min |
4. 1.3 mm/min |
5. 2.0 mm/min |
6. at Yield |
7. 80*10*3 sp=62mm |
8. 80*10*3 mm |
9. 80*10*4 mm |
10. 速率 A (50°C/h), 载荷2 (50N) |
11. 50 kW/m² |
【新闻资讯】查看全部
第二十届塑博会在余姚中塑国际会展中心举行
2018-11-12 11月7日-10日,第二十届中国塑料博览会(简称塑博会)在余姚中塑国际会展中心举行。本届塑博会以“创新、合作、共赢――迈向新时代”为主题,设置展出面积8个展馆7万平方米,展位3400个,设有塑料原料、塑料机械、模具机床、塑料制成品、智能机器人等5大展区。经过20年的发展,塑博会现已成为中国塑料行业具有知名度和影响力的品牌展会之一。 |
【免责声明】 广州搜料信息技术有限公司保留所有权利。 此数据表中的信息由搜料网soliao.com从该材料的生产商处获得。搜料网soliao.com尽最大努力确保此数据的准确性。 但是搜料公司对这些数据值及建议等给用户带来的不确定因素和后果不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。 |