Lexan BPL1000树脂Lexan BPL1000聚碳酸酯(PC)树脂是一种具有高流动性和良好冲击性能的注塑级树脂。它包含无氯化和无溴阻燃系统,UL-94V0额定值为0.8毫米。LEXAN™ BPL1000 resin提供各种不透明颜色选项,是薄壁应用的理想选择。 Lexan* BPL1000 Polycarbonate (PC) resin is an injection moldable grade featuring high flow and good impact peroformance. It contains non-chlorinated and non-brominated flame retardant systems with UL-94 V0 rating at 0.8mm. Lexan BPL1000 resin offers various opaque color options and is ideal for thin wall applications. |
技术参数 Technical Data | |||
---|---|---|---|
物理性能 PHYSICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
密度 Density |
1.17 | g/cm³ | ASTM D792 |
密度 Density |
1.20 | g/cm³ | ISO 1183 |
熔体质量流动速率 Melt Flow Rate |
|||
300℃,1.20kg 300℃,1.20kg |
25 | g/10min | ASTM D1238 |
熔体体积流动速率 Melt Volume Rate |
|||
300℃,1.2 kg 300℃,1.2 kg |
23.2 | cm³/10min | ISO 1133 |
收缩率 Shrinkage rate |
Internal Method | ||
MD MD 2 |
0.50 to 0.70 | % | 内部方法 |
MD:3.2 mm MD:3.2 mm |
% | 内部方法 | |
收缩率 Shrinkage rate |
|||
TD:3.2 mm TD:3.2 mm |
% | 内部方法 | |
吸水率 Water absorption rate |
|||
饱和,23℃ Saturation, 23 ℃ |
% | ISO 62 | |
平衡,23℃,50% RH Equilibrium, 23 ℃, 50% RH |
% | ISO 62 | |
机械性能 MECHANICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
拉伸模量 Tensile modulus 3 |
MPa | ASTM D638 | |
拉伸模量 Tensile modulus |
MPa | ISO 527-1-2 | |
拉伸强度 tensile strength |
|||
断裂 fracture 4 |
MPa | ASTM D638 | |
断裂 fracture |
MPa | ISO 527-2/50 | |
屈服 yield 4 |
MPa | ASTM D638 | |
屈服 yield |
MPa | ISO 527-2/50 | |
拉伸应变 Tensile strain |
|||
断裂 fracture 4 |
% | ASTM D638 | |
断裂 fracture |
% | ISO 527-2/50 | |
屈服 yield 4 |
% | ASTM D638 | |
屈服 yield |
% | ISO 527-2/50 | |
弯曲模量 Bending modulus 6 |
MPa | ISO 178 | |
50 mm跨距 50 mm span 5 |
MPa | ASTM D790 | |
弯曲强度 bending strength 6 , 7 |
MPa | ISO 178 | |
弯曲强度 bending strength 5 |
|||
屈服,50 mm跨度 Yield, 50 mm span 5 |
MPa | ASTM D790 | |
冲击性能 IMPACT |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
简支梁缺口冲击强度 Charpy Notched Impact Strength 8 |
|||
23℃ 23℃ 8 |
kJ/m² | ISO 179/1eA | |
悬臂梁缺口冲击强度 Impact strength of cantilever beam notch 9 |
ISO 180/1A | ||
23℃ 23℃ |
J/m | ASTM D256 | |
-30℃ -30℃ |
kJ/m² | ISO 180-1A | |
23℃ 23℃ |
kJ/m² | ISO 180-1A | |
装有测量仪表的落镖冲击 Dart impact equipped with measuring instruments |
|||
23℃,Total Energy 23℃,Total Energy |
J | ASTM D3763 | |
热性能 THERMAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
热变形温度 Hot deformation temperature |
|||
1.8 MPa,未退火,64 mm跨距 1.8 MPa, unannealed, 64 mm span 10 |
℃ | ISO 75-2/Af | |
0.45 MPa,未退火,3.2 mm 0.45 MPa, unannealed, 3.2 mm |
℃ | ASTM D648 | |
维卡软化温度 Vicat Softening Temp |
℃ | ASTM D1525 11 | |
维卡软化温度 Vicat Softening Temp |
|||
B50 B50 |
℃ | ISO 306 | |
B120 B120 |
℃ | ISO 306/B120 | |
球压测试 Ball pressure test |
|||
75℃ 75℃ |
IEC 60695-10-2 | ||
线性热膨胀系数 Linear coefficient of thermal expansion |
|||
TD:-40~40℃ TD:-40~40℃ |
1/℃ | ISO 11359-2 | |
TD:-40~40℃ TD:-40~40℃ |
1/℃ | ASTM E831 | |
MD:-40~40℃ MD:-40~40℃ |
1/℃ | ASTM E831 | |
MD:-40~40℃ MD:-40~40℃ |
1/℃ | ISO 11359-2 | |
相对温度指数 Relative temperature index |
|||
电气性能 Electrical performance |
℃ | UL 746 | |
强度机械性能 Strength mechanical performance |
℃ | UL 746 | |
冲击机械性能 Impact mechanical performance |
℃ | UL 746 | |
电气性能 Electrical performance |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
表面电阻率 Surface resistivity |
ohms | IEC 60093 | |
体积电阻率 Volume resistivity |
ohms·cm | IEC 60093 | |
介电强度 Dielectric strength |
|||
1.6 mm,在油中 1.6 mm in oil |
kV/mm | ASTM D149 | |
相对电容率 Relative permittivity |
IEC 60250 | ||
50 Hz 50 Hz |
IEC 60250 | ||
60 Hz 60 Hz |
IEC 60250 | ||
1 MHz 1 MHz |
IEC 60250 | ||
耗散因数 Dissipation factor |
IEC 60250 | ||
50 Hz 50 Hz |
IEC 60250 | ||
60 Hz 60 Hz |
IEC 60250 | ||
1 MHz 1 MHz |
IEC 60250 | ||
相比漏电起痕指数 Compared to the leakage tracing index |
V | IEC 60112 | |
阻燃性能 FLAME CHARACTERISTICS |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
阻燃等级 Flame retardant level |
UL 94 | ||
0.45 mm 0.45 mm |
UL 94 | ||
0.80 mm 0.80 mm |
UL 94 | ||
灼热丝可燃性指数 Glowing wire flammability index |
|||
1.0 mm 1.0 mm |
℃ | IEC 60695-2-12 | |
灼热丝起燃温度 Igniting temperature of the hot wire |
|||
1 mm 1 mm |
℃ | IEC 60695-2-13 | |
极限氧指数 Extreme oxygen index |
% | ISO 4589-2 |
备注 |
---|
1 一般属性:这些不能被视为规格。 |
2 Tensile Bar |
3 0,20 in/min |
4 类型 1, 2,0 in/min |
5 0,051 in/min |
6 0,079 in/min |
7 Yield |
8 80*10*4 sp=62mm |
9 80*10*4 |
10 80*10*4 mm |
11 标准 B (120°C/h), 载荷2 (50N) |
【新闻资讯】查看全部
废塑料化学回收市场前景向好
2021-12-13 搜料网资讯: 近年来,废塑料化学回收成为全球关注的话题。针对此,业内人士整理分析国内外科研和商业发展成果后指出,保守估计化学回收的潜在市场规模在万亿级别,预计2030年化 |
【免责声明】 广州搜料信息技术有限公司保留所有权利。 此数据表中的信息由搜料网soliao.com从该材料的生产商处获得。搜料网soliao.com尽最大努力确保此数据的准确性。 但是搜料公司对这些数据值及建议等给用户带来的不确定因素和后果不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。 |