牌号简介 About |
---|
中/高流量聚碳酸酯。用于医疗设备和医药应用。卫生保健变化管理,生物相容性(ISO10993或USP六级)。ETO和蒸汽灭菌。不含脱模剂。 Med/high flow polycarbonate. For medical devices and pharmaceutical applications. Healthcare management of change, biocompatible (ISO10993 or USP Class VI). EtO and steam sterilizable. Contains no mold release. |
技术参数 Technical Data | |||
---|---|---|---|
物理性能 PHYSICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
密度 Density |
|||
-- -- |
g/cm³ | ASTM D792 | |
-- -- |
1.19 | g/cm³ | ISO 1183 |
特定体积 Specific volume |
0.830 | cm³/g | ASTM D792 |
熔体质量流动速率 Melt Flow Rate |
|||
300℃,1.20kg 300℃,1.20kg |
18 | g/10min | ASTM D1238 |
熔体体积流动速率 Melt Volume Rate |
|||
300℃,1.2 kg 300℃,1.2 kg |
16.0 | cm³/10min | ISO 1133 |
收缩率 Shrinkage rate |
|||
MD:3.2 mm MD:3.2 mm |
0.50 到 0.70 | % | 内部方法 |
吸水率 Water absorption rate |
|||
24hr 24hr |
% | ASTM D570 | |
饱和,23℃ Saturation, 23 ℃ |
% | ISO 62 | |
平衡,23℃ Equilibrium, 23 ℃ |
% | ASTM D570 | |
平衡,100℃ Equilibrium, 100 ℃ |
% | ASTM D570 | |
平衡,23℃,50% RH Equilibrium, 23 ℃, 50% RH |
% | ISO 62 | |
冲击性能 IMPACT |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
简支梁缺口冲击强度 Charpy Notched Impact Strength |
|||
-30℃ -30℃ 8 |
kJ/m² | ISO 179/1eA | |
23℃ 23℃ 8 |
kJ/m² | ISO 179/1eA | |
23℃ 23℃ |
kJ/m² | ISO 179/2C | |
简支梁无缺口冲击强度 Charpy Unnotch Impact strength 8 |
|||
-30℃ -30℃ |
|||
23℃ 23℃ |
|||
悬臂梁缺口冲击强度 Impact strength of cantilever beam notch |
|||
23℃ 23℃ |
J/m | ASTM D256 | |
-30℃ -30℃ 9 |
kJ/m² | ISO 180-1A | |
23℃ 23℃ 9 |
kJ/m² | ISO 180-1A | |
悬臂梁无缺口冲击强度 Notched impact strength of cantilever beam |
|||
23℃ 23℃ |
J/m | ASTM D4812 | |
-30℃ -30℃ 9 |
ISO 180/1U | ||
23℃ 23℃ 9 |
ISO 180/1U | ||
装有测量仪表的落镖冲击 Dart impact equipped with measuring instruments |
|||
23℃,Total Energy 23℃,Total Energy |
J | ASTM D3763 | |
落锤冲击 Drop hammer impact |
|||
23℃ 23℃ |
J | ASTM D3029 | |
拉伸冲击强度 Tensile impact strength 10 |
kJ/m² | ASTM D1822 | |
热性能 THERMAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
热变形温度 Hot deformation temperature |
|||
0.45 MPa,未退火,6.4 mm 0.45 MPa, unannealed, 6.4 mm |
℃ | ASTM D648 | |
1.8 MPa,未退火,6.4 mm 1.8 MPa, unannealed, 6.4 mm |
℃ | ASTM D648 | |
1.8 MPa,未退火,100 mm跨距 1.8 MPa, unannealed, 100 mm span 11 |
℃ | ISO 75-2/Ae | |
维卡软化温度 Vicat Softening Temp |
|||
-- -- |
℃ | ASTM D1525 12 | |
B50 B50 |
℃ | ISO 306 | |
B120 B120 |
℃ | ISO 306/B120 | |
线性热膨胀系数 Linear coefficient of thermal expansion |
|||
MD:-40~95℃ MD:-40~95℃ |
1/℃ | ASTM E831 | |
MD:23~80℃ MD:23~80℃ |
1/℃ | ISO 11359-2 | |
TD:-40~95℃ TD:-40~95℃ |
1/℃ | ASTM E831 | |
TD:23~80℃ TD:23~80℃ |
1/℃ | ISO 11359-2 | |
比热 specific heat |
J/kg/℃ | ASTM C351 | |
导热系数 Thermal conductivity coefficient |
|||
-- -- |
W/m/K | ASTM C177 | |
-- -- |
W/m/K | ISO 8302 | |
相对温度指数 Relative temperature index |
℃ | UL 746 | |
电气性能 Electrical performance |
℃ | UL 746 | |
冲击机械性能 Impact mechanical performance |
℃ | UL 746 | |
电气性能 Electrical performance |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
表面电阻率 Surface resistivity |
ohms | IEC 60093 | |
体积电阻率 Volume resistivity |
|||
-- -- |
ohms·cm | ASTM D257 | |
-- -- |
ohms·cm | IEC 60093 | |
介电强度 Dielectric strength |
|||
3.2 mm,在空气中 3.2 mm in air |
kV/mm | ASTM D149 | |
3.2 mm,在油中 3.2 mm in oil |
kV/mm | IEC 60243-1 | |
介电常数 Dielectric constant |
|||
60 Hz 60 Hz |
ASTM D150 | ||
50 kHz 50 kHz |
ASTM D150 | ||
1 MHz 1 MHz |
ASTM D150 | ||
50 Hz 50 Hz |
IEC 60250 | ||
60 Hz 60 Hz |
IEC 60250 | ||
1 MHz 1 MHz |
IEC 60250 | ||
耗散因数 Dissipation factor |
|||
50 Hz 50 Hz |
ASTM D150 | ||
60 Hz 60 Hz |
ASTM D150 | ||
1 MHz 1 MHz |
ASTM D150 | ||
50 Hz 50 Hz |
IEC 60250 | ||
60 Hz 60 Hz |
IEC 60250 | ||
相比漏电起痕指数 Compared to the leakage tracing index |
UL 746 | ||
高电弧燃烧指数(HAI) High Arc Burning Index (HAI) 13 |
UL 746 | ||
高电压电弧起痕速率 High voltage arc marking rate |
|||
HVTR HVTR |
UL 746 | ||
热丝引燃 Hot wire ignition |
|||
HWI HWI |
UL 746 | ||
阻燃性能 FLAME CHARACTERISTICS |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
阻燃等级 Flame retardant level |
|||
1.50 mm 1.50 mm |
UL 94 | ||
极限氧指数 Extreme oxygen index |
% | ASTM D2863 | |
光学性能 optical performance |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
折射率 Refractive index |
ASTM D542 | ||
透光率 Transmittance |
|||
2540 µm 2540 µm |
% | ASTM D1003 | |
雾度 Haze |
|||
2540 µm 2540 µm |
% | ASTM D1003 | |
机械性能 MECHANICAL |
额定值 Nominal Value |
单位 Units |
测试方法 Test Method |
洛氏硬度 Rockwell hardness |
|||
M 级 M-level |
|||
R 级 R-level |
|||
拉伸模量 Tensile modulus |
|||
-- -- 3 |
MPa | ASTM D638 | |
-- -- |
MPa | ISO 527-1-2 | |
拉伸强度 tensile strength |
|||
屈服 yield 4 |
MPa | ASTM D638 | |
屈服 yield |
MPa | ISO 527-2/50 | |
断裂 fracture 4 |
MPa | ASTM D638 | |
断裂 fracture |
MPa | ISO 527-2/50 | |
拉伸应变 Tensile strain |
|||
屈服 yield 4 |
% | ASTM D638 | |
屈服 yield |
% | ISO 527-2/50 | |
断裂 fracture 4 |
% | ASTM D638 | |
断裂 fracture |
% | ISO 527-2/50 | |
弯曲模量 Bending modulus |
|||
50 mm跨距 50 mm span 5 |
MPa | ASTM D790 | |
-- -- 6 |
MPa | ISO 178 | |
弯曲强度 bending strength |
|||
-- -- 6 , 7 |
MPa | ISO 178 | |
屈服,50 mm跨度 Yield, 50 mm span 5 |
MPa | ASTM D790 | |
泰伯耐磨性 Taber abraser |
|||
1000 周期,1000 g,CS-17 转轮 1000 cycles, 1000 g, CS-17 wheels |
mg | ASTM D1044 |
备注 |
---|
3. 50 mm/min |
4. 类型 1, 50 mm/min |
5. 1.3 mm/min |
6. 2.0 mm/min |
7. at Yield |
8. 80*10*3 sp=62mm |
9. 80*10*3 mm |
10. Type S |
11. 120*10*4 mm |
12. 速率 A (50°C/h), 载荷2 (50N) |
13. Surface |
【新闻资讯】查看全部
朗盛:推出用于生产电池外壳的玻纤增强PA6
2021-08-26 搜料网资讯: 特殊化学品公司朗盛和韩国汽车零部件专家INFAC共同开发了一种用于电动汽车(EV)的电池模块外壳。 该电池外壳采用了朗盛的Durethan BKV30FN04,以满足最新的电动汽车部件 |
【免责声明】 广州搜料信息技术有限公司保留所有权利。 此数据表中的信息由搜料网soliao.com从该材料的生产商处获得。搜料网soliao.com尽最大努力确保此数据的准确性。 但是搜料公司对这些数据值及建议等给用户带来的不确定因素和后果不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。 |